Causes of Iron Inclusions on the Surface of Silica Sol Castings

Update On 2024-01

With the introduction of silica sol shell production technology in China, China's investment casting production has achieved rapid development and great progress. In response to the development of the casting industry in recent years, the competition within the industry has become more and more fierce. Comparisons are being made in terms of raw materials, equipment, craftsmanship, etc., and customers have higher and higher requirements for the quality of castings. Therefore, our company, Besser Casting also switched from water glass process to the silica sol process in 2008, and has made breakthroughs and innovations in some technologies.

 

Due to limited space and experience, only the bits and pieces of experience that came from the practice in production and achieved practical results are summarized. If you have other opinions, you are welcome to write them down in the comment area.

 

There are many reasons for iron clamping in castings, which can be analyzed from the three aspects: welding, shell making and casting. Among the three, shell making is the most critical. Therefore, first we analyze the causes of iron clamping from the aspect of shell making:

Cause 1
If the mixing of raw materials is improper, a large amount of gas generated by chemical reactions in the surface slurry will attach to the wax parts along with the paint. In addition, if the slurry is too thick, its fluidity will decrease. Therefore, some grooves and corners of the wax parts cannot be covered, leaving pores. Later, iron beans will appear after casting.

Countermeasure 1
Add an appropriate amount of defoamer and wetting agent when preparing the slurry. Notice that stirring requires sufficient time for the gas to escape. In addition, the spraying dilute coating method and spraying silica sol method can also reduce the iron bean phenomenon to a certain extent: 1) add silica sol to dilute the silica sol coating to a viscosity of 8-10s (0.3% wetting agent and 0.05% defoamer have been added); 2) put it into the spray gun, spray the wax mold on the bubble-prone area before dipping the wax, and then immerse it in the paint; 3) after taking it out, rotate it to ensure that the slurry does not accumulate, and blow it with an air gun. This method can eliminate "iron beans" defect.

Cause 2
The choice of sand grain mesh is incorrect. The structure of the casting is complex, with deep or narrow gaps or holes. If the sand is too thick, these places are plugged, making the dipping insufficient. As a result in shells are not dense, with thinner shells in some places, and reduced strength.


Countermeasure 2
Before dipping the slurry, use an air gun to blow off the floating sand on the upper layer. Then then pass the silica sol first, before dipping the slurry, which can enhance the fluidity of the slurry and prevent clogging. After the sand is floating, the operator can use a thin rod to pass through a round hole and the pile of sand at the gap, which is also conducive to the subsequent immersion of sand. In addition, for deep-hole products, the holes can be grouted and filled with sand after three layers to prevent iron leakage on the inner wall of the deep hole.
 


Cause 3
The mold shell is dry and impermeable, which will directly cause the strength of the shell to drop greatly. The ultimate cause is poor temperature and humidity in the workshop, which makes the drying time insufficient.The mold shell is dry and impermeable, which will directly cause the strength of the shell to drop greatly. The ultimate cause is poor temperature and humidity in the workshop, which makes the drying time insufficient.
Countermeasure 3
Control the temperature and humidity of the workshop, the specific values are as follows, adjusted according to the actual situation:
 
Number of layersTemperatureHumidityViscosityWind speedDrying time
Surface layer22±2℃60-80%35-45snone>4h
Second layer24±2℃50-60%15-25s2-4m/s>6h
After the third
layer
26±2℃40±10%10-15s>6m/s>8h
 

Note that the surface layer should not be too dry, otherwise it will cause the casting to bulge. A humidifier can be placed between the surface layers to maintain humidity. For different product structures, the drying time is different. We need to plan the parking time in the workshop scientifically and reasonably. For this reason, Besser Casting has also specially equipped with humidity detectors and anemometers to help employees judge whether the mold shell is dry.


Next, let’s talk about welding. It does not directly lead to iron clamping in the product. However, due to the unreasonable welding process, it will increase the difficulty of the shell making operation. As a result, the iron clamping rate of the product will increase. In order to maximize the benefits, it’s common for factories to assemble full products on a square die. However, although the production rate is high, the product group is too dense, which will prevent the grout sand from entering. The thickness of the shell between the gate and the wax rod is not enough. Without a certain strength, the molten steel will leak when it is flushed by molten steel. Therefore, the gap between the products should be arranged reasonably. Besides, for products with deep-hole grooves, the complex side must face up or back to the wax stick, so as to facilitate leaching, blowing and drying. The salaries of shell workers are based on the number of products they make. They cannot waste too much time and energy on a series of products. For them, the more they do in the same time, the more they take. Thereby, we should also improve the welding method so as to help them reduce the difficulty of operation, improve work efficiency, and ensure product quality.


The last thing to talk about is casting. Cast iron is mainly manifested as molten steel. The reason is that the mold shell is cracked. Improper dewaxing operation and collision during handling will cause the mold shell to crack before casting. Therefore, it is also necessary to strengthen the skill training of the dewaxing workers, and the furnace workers to inspect the mold shells before firing. If there are broken parts and cracks, they should be repaired in time. In addition, the molten steel is too heavy, and the mold shell cannot bear the weight, which will cause cracks. This involves the improvement of the welding process.





Related content recommendation

Qianhao Foundry is the top custom investment casting manufacturer in China. We can supply all kinds of different investment casting parts in steel, carbon steel, alloy steel, etc. Pls contact us if you have any need for investment casting solution!
Conatct Us
Contact Us
Ningbo Qianhao Metal Product Co.,LTD
No.2086 Ningheng South Road, Hengxi Town,Yinzhou,Ningbo,315131,Zhejiang ,China
sale@lx8.cn
Copyright © Ningbo Qianhao Metal Product Co.,LTD All Rights Reserved | www.lostwaxcasting-china.com | Sitemap